Specifications
PropertyValueUnit
Physical Properties
Density1.5ISO 1183- 23°Cg/mL
Shrinkage0.3ISO 294-4, 2 mm, Flow%
Melting point340ISO 11357, DSC - 2nd heating°C
Melting range380 – 400°C
Shrinkage0.6ISO 294-4, 2 mm, Transverse%
Processing Properties
MFI3380°C/5 kg- ISO 1133g/10min
Mold Temperature160 – 200°C
Die Temperature400°C
Drying Temperature160°C
Dry Time240min
Mechanical Properties
Tensile Stress at yield-MD165ISO 527-1MPa
Strain at break-MD2ISO 527-2%
Charpy Impact Strength (notched)10ISO 179/1eA, 23°C, Complete breakkJ/m2
(Charpy Impact Strength(unnotched70ISO 179/1eU, 23°C, Complete BreakkJ/m2
Tensile modulus-MD11,000MPa
(Charpy Impact Strength(unnotched75ISO 179/1eU, -30°C, Complete BreakkJ/m2
Charpy Impact Strength (notched)9ISO 179/1eA, -30°C, Complete break
Thermal Properties
Heat Deflection temperature335ISO 75-1, 0.45 MPa, Method B°C
Vicat softening temperature340ISO 306, 10N, Method A°C
FlameabilityV-0 ClassUL 94, 1.6 mm
Glass transition Temperature152°C
Heat Deflection temperature312ISO 75-1, 1.8 MPa, Method A°C
Vicat softening temperature335ISO 306, 50N, Method B°C
Chemical Properties
(LOI) Loss on ignition45ISO 4589, 3.2 mm%
Water absorption0.4ISO 62, 23°C, Saturation%
Electrical Properties
Surface Resistance10^14IEC 60093ohm
Volume resistance10^15×10^11IEC 60093ohm-cm
Dissipation Factor0.004IEC 60250, 1 MHz
Comparative Tracking Index200IEC 60112, Test solution AV
Relative permittivity3.3IEC 60250, 1 MHz
Appearance Properties
Physical stateقرصی شکل